Skip to content

Joints

Reviewed by licensed engineers

Checked against its sources by licensed professional engineers on the previous site, where reviewers weren’t recorded by name.

How articles are reviewed

Joints are purposefully placed discontinuities in a rigid pavement surface course. All types of joints are used in rigid pavement construction methods for all PCC pavement types. CRCP uses longitudinal reinforcing steel in order to limit the number of transverse contraction joints, but it still uses longitudinal joints and periodic transverse joints.

Joints can be formed in two ways. Contraction joints are most often sawed in after PCC placement. Others such as expansion, isolation and construction joints, are created by formwork before the PCC is placed. Each one of these methods of joint construction has its own method and set of considerations.

Types

Contraction Joints

A contraction joint is a sawed, formed, or tooled groove in a concrete slab that creates a weakened vertical plane. It regulates the location of the cracking caused by dimensional changes in the slab. Unregulated cracks can grow and result in an unacceptably rough surface as well as water infiltration into the base, subbase and subgrade, which can enable other types of pavement distress. Contraction joints are the most common type of joint in concrete pavements, thus the generic term "joint" generally refers to a contraction joint.

Contraction joints are chiefly defined by their spacing and their method of load transfer. They are generally between 1/4 - 1/3 the depth of the slab and typically spaced every 3.1 - 15 m (12 - 50 ft.) with thinner slabs having shorter spacing (see Figure 1). Some states use a semi-random joint spacing pattern to minimize their resonant effect on vehicles. These patterns typically use a repeating sequence of joint spacing (for example: 2.7 m (9 ft.) then 3.0 m (10 ft.) then 4.3 m (14 ft.) then 4.0 m (13 ft.)). Transverse contraction joints can be cut at right angles to the direction of traffic flow or at an angle (called a "skewed joint", see Figure 3). Skewed joints are cut at obtuse angles to the direction of traffic flow to help with load transfer. If the joint is properly skewed, the left wheel of each axle will cross onto the leave slab first and only one wheel will cross the joint at a time, which results in lower load transfer stresses (see Figure 4).

Rigid Pavement Showing Contraction JointsMissing Contraction Joint (The middle lane contraction joint was not sawed resulting in a transverse slab crack. The outer lanes have proper contraction joints and therefore, no cracking)
Figures 1 and 2. Rigid Pavement Showing Contraction Joints Missing Contraction Joint (The middle lane contraction joint was not sawed resulting in a transverse slab crack. The outer lanes have proper contraction joints and therefore, no cracking)
Skewed Contraction Joint (The Tining is Perpendicular to the Direction of Travel While the Contraction Joint is Skewed)
Figure 3. Skewed Contraction Joint (The Tining is Perpendicular to the Direction of Travel While the Contraction Joint is Skewed)

Expansion Joints

An expansion joint is placed at a specific location to allow the pavement to expand without damaging adjacent structures or the pavement itself. Up until the 1950s, it was common practice in the U.S. to use plain, jointed slabs with both contraction and expansion joints (Sutherland, 1956). However, expansion joint are not typically used today because their progressive closure tends to cause contraction joints to progressively open (Sutherland, 1956). Progressive or even large seasonal contraction joint openings cause a loss of load transfer particularly so for joints without dowel bars.

Isolation Joints

An isolation joint (see Figure 5) is used to lessen compressive stresses that develop at T- and unsymmetrical intersections, ramps, bridges, building foundations, drainage inlets, manholes, and anywhere differential movement between the pavement and a structure (or another existing pavement) may take place (ACPA, 2001). They are typically filled with a joint filler material to prevent water and dirt infiltration.

Roofing Paper Used for an Isolation JointRoofing Paper Used for an Isolation Joint
Figures 4 and 5. Roofing Paper Used for an Isolation Joint Roofing Paper Used for an Isolation Joint

Construction Joints

A construction joint (see Figure 6) is a joint between slabs that results when concrete is placed at different times. This type of joint can be further broken down into transverse and longitudinal construction joints (see Figure 7). Longitudinal construction joints also allow slab warping without appreciable separation or cracking of the slabs.

Construction Joint
Figure 6. Construction Joint

Workers manually insert dowel bars into the construction joint at the end of the work day. Construction joints should be planned so that they coincide with contraction joint spacing to eliminate extra joints.

Longitudinal and Transverse Construction Joints
Figure 7. Longitudinal and Transverse Construction Joints

Teaching this? Figures and worked examples are free to use with credit. How to cite

Cite this page

APA

Pavement Interactive. (2021, March 5). Joints. HeadLight. Retrieved [the date you read it], from https://pavementinteractive.org/reference-desk/construction/placement/joints/

ASCE

Pavement Interactive. (2021). “Joints.” HeadLight, <https://pavementinteractive.org/reference-desk/construction/placement/joints/> ([the date you read it]).

BibTeX

@misc{pavint-joints,
  author = {{Pavement Interactive}},
  title = {Joints},
  year = {2021},
  publisher = {HeadLight},
  howpublished = {\url{https://pavementinteractive.org/reference-desk/construction/placement/joints/}},
  note = {Accessed [date]}
}
This address will not change. The citation records the date you read it.
Report an error

Reports go to the editors, who check them against the cited sources. Corrections are noted at the top of the article.

Only if you want a reply. It is not published.